| Departments | |
|---|---|
| Book Series (99) |
1420
|
| Nachhaltigkeit |
3
|
| Gesundheitswesen |
3
|
| Humanities |
2423
|
| Natural Sciences |
5433
|
| Engineering |
1827
|
| Engineering | 292 |
| Mechanical and process engineering | 876 |
| Electrical engineering | 702 |
| Mining and metallurgy | 30 |
| Architecture and civil engineering | 76 |
| Common |
97
|
|
Leitlinien Unfallchirurgie
5. Auflage bestellen |
|
The mechanical degradation behaviour of matrix dominated, continuous
±45◦ carbon fibre reinforced epoxide laminates from HTA/6376 prepregs
has been examined with particular regard to integrated load-property inter-
actions.
The mechanisms of deformation and damage evolution were assessed by
different experimental techniques such as stress-strain hysteresis measure-
ments, microscopy and thermography. The fibre rotation effect was found to
be negligible for all loadings.
With respect to the statistically distributed damage evolution, homogenised
strain based approaches were developed and successfully applied to the pre-
dict strength and life time under static and cyclic loads. The material focus
was directed towards, first the dependence of the (quasi-static and cyclic)
material response on the load rate, second, the interaction of creep and fa-
tigue, and third, the influence of load sequences and pre-loads in fatigue. The
main findings are:
1. The quasi-static stress-strain behaviour exhibits a characteristic yield-
ing with a load rate dependence. With increasing strain rate, the lam-
inate becomes stiffer, stronger, and more brittle. The distribution of
material defects does not affect stiffness and yield properties but de-
termines whether the rupture process is dominated by local or global
energy dissipation.
2. A threshold stress value for static creep could be determined and a
parametric function to predict the stress and time dependent strain
evolution given. Cyclic creep occurs once the mean stress in fatigue
exceeds the threshold stress for static creep. The portions of creep and
fatigue strain to the total strain under cyclic loading could be separated
and well estimated.
3. The fatigue life and the damage accumulation behaviour under block
load conditions are dependent on the load sequence and the load level.
Strain based damage accumulation approaches could be developed and
verified for different load sequences.
Pre-loads (initial pulse or cyclic stresses, or creep and recovery) tend to
prolong the subsequent fatigue life. This effect is believed to result from
the reduction of stress intensities in the matrix by plastic deformation.
The plastic deformations due to initial loads and due to cyclic creep
are thereby competitive.
| ISBN-13 (Printausgabe) | 3865370241 |
| ISBN-13 (Hard Copy) | 9783865370242 |
| ISBN-13 (eBook) | 9783736910249 |
| Language | German |
| Page Number | 204 |
| Edition | 1 |
| Volume | 0 |
| Publication Place | Göttingen |
| Place of Dissertation | Göttingen |
| Publication Date | 2004-03-11 |
| General Categorization | Dissertation |
| Departments |
Mechanical and process engineering
|
| Keywords | Carbon Fibre Reinforced Polymers (CFRP), Angle-Ply Composite Laminates, Static and Cyclic Loading, Fatigue Life, Creep Behaviour, Creep-Fatigue Interaction, Mechanical Damage Evolution, Strain Rate Dependence, Stress-Strain Behaviour, Damage Accumulation, Load Sequence Effects, Pre-Loading Effects, Fatigue Life Prediction, Strain-Based Damage Models, Infrared Thermography |